PWHT 580°C 1h | |||||
Elongation | Tensile Strength | Yield Strength | 保护气体 | Stress Relieved Temperature | Stress Relieved Testing Time |
21 % | 710 MPa | 650 MPa | ISO | - | - |
Stress relieved | |||||
Elongation | Tensile Strength | Yield Strength | 保护气体 | Stress Relieved Temperature | Stress Relieved Testing Time |
- | - | - | AWS | 620 °C | 1 hr |
PWHT 580°C 1h | ||
Impact Value | Testing Temperature | 保护气体 |
80 J | -50 °C | ISO |
60 J | -60 °C | ISO |
Mn | |||||
Mn | Mo | C | Si | Ni | Cr |
1.85 % | - | - | - | - | - |
Mo | |||||
Mn | Mo | C | Si | Ni | Cr |
- | 0.32 % | - | - | - | - |
C | |||||
Mn | Mo | C | Si | Ni | Cr |
- | - | 0.06 % | - | - | - |
Si | |||||
Mn | Mo | C | Si | Ni | Cr |
- | - | - | 0.35 % | - | - |
Ni | |||||
Mn | Mo | C | Si | Ni | Cr |
- | - | - | - | 0.89 % | - |
Cr | |||||
Mn | Mo | C | Si | Ni | Cr |
- | - | - | - | - | 0.05 % |
Fusion time per electrode at 90% I max | kg weld metal/kg electrodes | Number of electrodes/kg weld metal | 安培 | 熔敷率 | 电压 V | 直径 |
60 sec | 0.60 kg | 83.3 | 55-85 A | 0.72 kg/h | 24.4 V | 2.5 x 350 mm |
68 sec | 0.55 kg | 56.6 | 80-140 A | 0.94 kg/h | 23.3 V | 3.2 x 350 mm |
103 sec | 0.60 kg | 24.4 | 120-180 A | 1.43 kg/h | 24.0 V | 4.0 x 450 mm |